Technical Data
Ti-6Al-2Zr-2Sn-2Mo-2Cr-0.25Si (Ti-6-22-22)
Ti-6-22-22 was developed for high strength, deep hardenable and high toughness.
Chemistry Limits (%) |
|
Al | 5.5 - 6.5 |
Sn | 1.5 - 2.5 |
Zr | 1.5 - 2.5 |
Mo | 1.5 - 2.5 |
Cr | 1.5 - 2.5 |
Cr + Mo | 4.0 - 5.0 |
Si | 0.2 - 0.3 |
O2 Max | 0.14 |
H2 Max | 0.01 |
C Max | 0.05 |
N2 Max | 0.04 |
Mechanical Properties |
|
Typicals |
Solution Treated and Aged Condition (STA) |
Ultimate Tensile Strength - ksi | 186 |
Yield Strength - ksi | 165 |
Elongation % | 11 |
Physical Properties |
|
Density (lbs/in3) | 0.168 |
Elastic Modulus (x106 psi) | 17.7 |
Beta Transus Temp (oF) | 1760 |
Weldability | Not Recommended |